耐火材料 ›› 2025, Vol. 59 ›› Issue (5): 406-412.DOI: 10.3969/j.issn.1001-1935.2025.05.007

• 研究开发 • 上一篇    下一篇

基于固溶途径的高纯超细Ti3(Al1.2-xSnx)C2粉末制备及其力学性能研究

吴沛宸, 王璐, 李洞亭, 刘颖   

  1. 四川大学 材料科学与工程学院 四川成都 610065
  • 收稿日期:2024-12-05 出版日期:2025-10-15 发布日期:2025-10-22
  • 通讯作者: 刘颖,男,1965年生,博士,教授。 E-mail:liuying5536@scu.edu.cn
  • 作者简介:吴沛宸:男,2000年生,硕士研究生。E-mail:wpc2410361097@163.com

Preparation of high-purity ultrafine Ti3(Al1.2-xSnx)C2 powder and its mechanical properties based on solid solution route

Wu Peichen, Wang Lu, Li Dongting, Liu Ying   

  1. First auther's address:College of Materials Science and Engineering,Sichuan University,Chengdu 610065,Sichuan,China
  • Received:2024-12-05 Online:2025-10-15 Published:2025-10-22

摘要: 随着服役工况的恶劣和对部件性能要求的提高,单相Ti3AlC2陶瓷因低韧性和低耐磨性短板,已难以契合现代工业装备愈发严苛的要求。发展有效手段可控制备高纯度、小粒径的Ti3AlC2固溶体粉末,并制备出具有较好综合力学性能的Ti3AlC2固溶体材料刻不容缓。运用固溶途径,将Ti、Al、Sn、TiC粉末置于行星球磨机内混合,采用两步无压烧结法与机械球磨法制备了高纯超细的Ti3(Al1.2-xSnx)C2 (x分别为0、0.1、0.3和0.5) 粉末,并经放电等离子烧结制备了Ti3(Al1.2-xSnx)C2块状试样。结果表明:Ti3(Al1.2-xSnx)C2 (x分别为0、0.1、0.3 和0.5) 粉末纯度均>99%(w),且呈现出纳米层状结构;放电等离子烧结制备的Ti3(Al1.2-xSnx)C2试样随着Sn固溶量的增加,力学性能均有较大提升,其中维氏硬度、抗弯强度、断裂韧性及抗压强度均呈现先增大后减小的趋势,Ti3(Al0.9Sn0.3)C2试样的力学性能最好,维氏硬度、抗弯强度、断裂韧性和抗压强度分别为8.38 GPa、820.91 MPa、7.87 MPa·m1/2和1 510 MPa;Ti3(Al1.2-xSnx)C2材料强度与硬度的提升在于固溶强化与第二相强化,而材料的分层结构、裂纹扩展的偏转及断裂面的晶粒拉出等微观特性,协同增强了材料的抗变形与断裂能力。

关键词: Ti3(Al1.2-xSnx)C2, 固溶强化, 无压烧结, 放电等离子烧结, 力学性能

Abstract: As service conditions become harsh and performance requirements for components increase,single-phase Ti3AlC2 ceramics are difficult to meet the increasingly stringent requirements of modern industrial equipment because of their short comings of low toughness and poor wear resistance.It is urgent to develop effective methods for the controllable preparation of high-purity and small-particle size Ti3AlC2 solid solution powder and to fabricate Ti3AlC2 solid solution materials with good comprehensive mechanical properties.High-purity ultrafine Ti3(Al1.2-xSnx)C2(x=0,0.1,0.3 and 0.5) powders were prepared by mixing Ti,Al,Sn and TiC powders through the solid solution route in a planetary ball mill,two-step pressureless sintering and mechanical ball milling.Ti3(Al1.2-xSnx)C2 bulk samples were then prepared by spark plasma sintering.The results show that all the Ti3(Al1.2-xSnx)C2(x=0,0.1,0.3 and 0.5) powders have a purity of >99 mass% as well as a nano-layered structure.The mechanical properties of the Ti3(Al1.2-xSnx)C2 samples prepared by spark plasma sintering are greatly improved with the increase of the Sn solid solution,among which the Vickers hardness,bending strength,fracture toughness and compressive strength all increase first and then decrease.Sample Ti3(Al0.9Sn0.3)C2 has the best mechanical properties,with the Vickers hardness of 8.38 GPa,bending strength of 820.91 MPa,fracture toughness of 7.87 MPa·m1/2 and compressive strength of 1 510 MPa.The improvement of the strength and hardness of Ti3(Al1.2-xSnx)C2 materials lies in solid solution strengthening and second phase strengthening,and the micro-characteristics of the materials,such as the layered structure,deflection of crack propagation and grain pull-out of the fracture surface,enhance the deformation and fracture resistance of the materials cooperatively.

Key words: Ti3(Al1.2-xSnx)C2, solid solution strengthening, pressureless sintering, spark plasma sintering, mechanical properties

中图分类号: