耐火材料 ›› 2025, Vol. 59 ›› Issue (5): 427-431.DOI: 10.3969/j.issn.1001-1935.2025.05.010

• 生产应用 • 上一篇    下一篇

片状氮化硅陶瓷的水基流延成型制备工艺研究

赵辰啸1), 李世鹏1), 王刚1), 袁波2)   

  1. 1)中钢集团洛阳耐火材料研究院有限公司 先进耐火材料全国重点实验室 河南洛阳 471039
    2)上海大学 先进耐火材料全国重点实验室 上海 200444
  • 收稿日期:2025-01-17 出版日期:2025-10-15 发布日期:2025-10-22
  • 通讯作者: 袁波,男,1983年生,博士,正高级工程师。 E-mail:boyuan0401@163.com
  • 作者简介:赵辰啸:男,2000年生,硕士研究生。E-mail:15530090311@163.com

Preparation process of water based tape casting of plate-like silicon nitride ceramics

Zhao Chenxiao, Li Shipeng, Wang Gang, Yuan Bo   

  1. First author's address:State Key Laboratory of Advanced Refractories,Sinosteel Luoyang Institute of Refractories Research Co.,Ltd.,Luoyang 471039,Henan,China
  • Received:2025-01-17 Online:2025-10-15 Published:2025-10-22

摘要: 为制备无明显变形且成本低、性能良好的片状氮化硅陶瓷,以α-Si3N4粉为原料,以LiAlO2粉、Y2O3粉为烧结助剂,去离子水为溶剂,以四甲基氢氧化铵为分散剂,以亚克力树脂乳液为黏结剂,以水溶性低聚物为增塑剂,制备了固相体积分数为45%的氮化硅水基浆料。研究了分散剂加入量(质量分数为0.1%~0.9%,间隔0.1%)、球磨时间(1、3、5、7 h)、黏结剂加入量(质量分数2.5%、5.0%、7.5%)、增塑剂与黏结剂的质量比(0、0.3、0.6、0.9)等因素对浆料性能和流延效果的影响。结果发现,当分散剂、黏结剂的加入量(w)分别为0.6%、7.5%,增塑剂与黏结剂的质量比为0.6,低速球磨时间为5 h时,固相体积分数为45%的氮化硅水基浆料的流动性和流延效果最好。以此浆料进行流延、干燥、叠压,制得片状氮化硅陶瓷素坯,再在氮气气氛经 1 650 ℃常压烧结3 h,得到片状氮化硅陶瓷,其相对密度为97.12%,硬度为15.64 GPa,抗弯强度和断裂韧性分别为 583.58 MPa和6.72 MPa·m1/2

关键词: 氮化硅陶瓷, 固含量, 水基流延成型, 常压烧结

Abstract: To prepare plate-like silicon nitride ceramics with minimal deformation,low cost,and excellent performance,a water based silicon nitride slurry with a solid loading of 45 vol% was prepared using α-Si3N4 powder as the raw material,LiAlO2 powder and Y2O3 powder as the sintering aids,deionized water as the solvent,tetramethyl ammonium hydroxide as the dispersant,acrylic resin emulsion as the binder,and water-soluble oligomer as the plasticizer.The influence of factors such as the dispersant addition (0.1%-0.9%,at an interval of 0.1%,by mass),ball milling time (1,3,5 and 7 h),binder addition (2.5%,5.0% and 7.5%,by mass),and mass ratio of plasticizer to binder (0,0.3,0.6 and 0.9) on the properties and tape casting effect of the slurry was studied.The results show that with the dispersant addition of 0.6%,the binder addition of 7.5%,the mass ratio of plasticizer to binder of 0.6 and the low speed ball milling time of 5 h,the water based silicon nitride slurry with a solid loading of 45% performs the best flowability and tape casting effect.Using this slurry for tape casting,drying,and laminating,plate-like silicon nitride ceramic green bodies were obtained.Then,they were pressureless sintered at 1 650 ℃ for 3 h in a nitrogen atmosphere to obtain plate-like silicon nitride ceramics.The ceramics have the relative density of 97.12%,hardness of 15.64 GPa,bending strength of 583.58 MPa and fracture toughness of 6.72 MPa·m1/2.

Key words: silicon nitride ceramics, solid loading, water based tape casting, pressureless sintering

中图分类号: