Refractories ›› 2026, Vol. 60 ›› Issue (5): 376-382.DOI: 10.3969/j.issn.1001-1935.2026.05.002

Previous Articles     Next Articles

Effect of zircon on sintering behavior and alkali corrosion resistance of bauxite-based mullite homogeneous grogs

Zhao Fei, Li Ruoxi, Wang Yali, Mai Haixiang, Zuo Yudong, An Jiancheng, Lian Weikang   

  1. First author’s address:Henan Key Laboratory of High Temperature Functional Ceramics,Zhengzhou University,Zhengzhou 450052,Henan,China
  • Received:2025-12-29 Online:2026-10-15 Published:2026-10-29

锆英石对矾土基莫来石均质料烧结行为及抗碱侵蚀性的影响

赵飞1), 李若茜1), 王亚利2,3), 麦海香1), 左玉冬1), 安建成2,3), 连伟康1,2)   

  1. 1)郑州大学 河南省高温功能材料重点实验室 河南郑州 450052
    2)阳泉金隅通达高温材料有限公司 山西阳泉 045000
    3)北京金隅通达耐火技术有限公司 北京海淀 100096
  • 作者简介:赵飞:男,1982年生,博士,高级工程师。E-mail:zhaofeiln@zzu.edu.cn
  • 基金资助:
    2024年度山西省中央引导地方科技发展资金项目(YDZJSX2024C032)。

Abstract: To improve the alkali corrosion resistance of bauxite-based mullite homogeneous grogs,a series of ZrO2-doped bauxite-based mullite homogeneous grogs were prepared by wet mixing,shaping and calcining at 1 350-1 650 ℃ for 4 h,using grade Ⅱ high-alumina bauxite as the main raw material and zircon as the modifying additive.The effects of varying zircon additions (0,2%,4%,and 6%,by mass) on the sintering behavior,phase composition,and cold physical properties of the grogs were investigated,and their alkali corrosion resistance was evaluated by the static crucible method.The results indicate that between 1 450 and 1 650 ℃,SiO2 generated from zircon decomposition forms a SiO2-rich liquid phase at the ZrO2 interface,which accelerates the sintering shrinkage of the mullite homogeneous grogs.Concurrently,a portion of this SiO2-rich liquid phase participates in the mullitization reaction during calcination and is consumed in situ.ZrO2 decomposed from zircon is dispersively distributed in the glass phase and at mullite grain boundaries,increasing the viscosity of the glass phase.After calcination at 1 650 ℃,the apparent porosity of the homogeneous grogs decreases from 0.63% to 0.20% with the increase of zircon addition.Furthermore,the increased ZrO2 addition inhibits the diffusion and penetration rate of K+ in alkaline corrosion environments,thereby improving the alkali corrosion resistance of the bauxite-based mullite homogeneous grogs.When the zircon addition is 4%,the sample calcined at 1 650 ℃ for 4 h exhibits high density,excellent cold mechanical properties and favorable alkali corrosion resistance.

Key words: bauxite, zircon, bauxite-based mullite homogeneous grogs, alkali corrosion resistance

摘要: 为提升矾土基莫来石均质料的抗碱侵蚀性能,以Ⅱ级高铝矾土为主要原料,锆英石为改性添加剂,经湿混、成型、1 350~1 650 ℃保温4 h煅烧制备了系列ZrO2掺杂矾土基莫来石均质料,研究了锆英石加入量(加入质量分数分别为0、2%、4%和6%)对其烧结特性、物相组成及常温物理性能的影响,并采用静态坩埚法评估其抗碱侵蚀性能。结果表明:1 450~1 650 ℃煅烧后,锆英石分解产生的SiO2在ZrO2界面形成富SiO2液相,该液相可加快莫来石均质料的烧结收缩进程。同时,部分富SiO2液相在煅烧过程中参与莫来石化反应并被原位消耗。锆英石分解产物ZrO2以弥散态分布于均质料的玻璃相及莫来石晶界处,提高了玻璃相的黏度。经1 650 ℃煅烧后,随着锆英石加入量的增加,均质料的显气孔率从0.63%降至0.20%,且增加ZrO2加入量可抑制碱蚀环境中K+的扩散与渗透,从而提升莫来石均质料的抗碱侵蚀性能。当锆英石加入量为4%(w)时,1 650 ℃保温4 h煅烧后试样兼具高致密度、优异的常温力学性能与良好的抗碱侵蚀性能。

关键词: 铝矾土, 锆英石, 矾土基莫来石均质料, 抗碱侵蚀性能

CLC Number: