耐火材料 ›› 2022, Vol. 56 ›› Issue (2): 101-106.DOI: 10.3969/j.issn.1001-1935.2022.02.002

• 研究开发 • 上一篇    下一篇

模板浸渍法制备ZrO2纤维研究

张雷(), 闫森旺, 李虹屿, 孙小飞(), 王刚, 张一帆, 王守业   

  1. 中钢集团洛阳耐火材料研究院有限公司 先进耐火材料国家重点实验室 河南洛阳 471039
  • 收稿日期:2021-08-17 出版日期:2022-04-15 发布日期:2022-04-21
  • 通讯作者: 孙小飞,男,1981年生,博士,教授级高级工程师。E-mail: sunxiaofei0217@163.com
  • 作者简介:张雷:男,1994年生,硕士研究生。E-mail: 937268721@qq.com
  • 基金资助:
    国家重点研发计划资助项目(2018YFB0605904)

Preparation of ZrO2 fibers by template impregnation method

Zhang Lei(), Yan Senwang, Li Hongyu, Sun Xiao-fei(), Wang Gang, Zhang Yifan, Wang Shouye   

  1. State Key Laboratory of Advanced Refractories,Sinosteel Luoyang Institute of Refractories Research Co.,Ltd.,Luoyang 471039,Henan,China
  • Received:2021-08-17 Online:2022-04-15 Published:2022-04-21
  • Contact: Sun Xiao-fei

摘要:

将15 cm×15 cm×1 cm的粘胶纤维模板放入浓度为1、2及3 mol·L-1的ZrOCl2溶液,分别在20、40、60 ℃下浸渍20 h,经过洗涤、离心、干燥得到ZrO2纤维前驱体,再对前驱体进行600、800、1 000、1 200 ℃保温 2 h热处理制得ZrO2纤维。研究浸渍温度、浸渍液浓度、热处理温度对ZrO2纤维形貌和相组成的影响。结果表明,随着浸渍温度由20 ℃提高到60 ℃,浸渍液浓度由1 mol·L-1提高到3 mol·L-1,纤维横截面微观形貌由扁平状向圆柱状变化,同时纤维的平均直径逐渐增大,说明提高浸渍温度和浸渍液浓度有利于粘胶纤维模板对Zr4+的吸附。ZrO2纤维经过热处理后,主要是以单斜相ZrO2存在。随着热处理温度的增加,ZrO2纤维晶粒变大,结晶程度增加,同时纤维表面经历由光滑到小晶粒出现再到裂纹出现的转变。

关键词: ZrO2纤维, 模板浸渍法, 显微形貌, 直径

Abstract:

Viscose fiber templates (15 cm×15 cm×1 cm) were put into ZrOCl2 solutions of different concentrations (1,2 and 3 mol·L-1) and impregnated at 20,40 and 60 ℃ for 20 h,respectively.After washing,centrifugation and drying,ZrO2 fiber precursors were obtained.ZrO2 fibers were prepared by heat treatment of the precursors at 600,800,1 000 and 1 200 ℃ for 2 h.The effects of the impregnation temperature,the impregnation solution concentrations and the heat treatment temperature on the microstructure and the phase composition of the ZrO2 fibers were studied.The results show that with the increase of the impregnation temperature from 20 ℃ to 60 ℃ and the impregnation solution concentration increases from 1 mol·L-1 to 3 mol·L-1,the microstructure of fiber cross section changes from flat to cylindrical,and the average fiber diameter increases,indicating that the increase of the impregnation solution concentration and the impregnation temperature is beneficial to increasing the adsorption capacity of Zr4+ on viscose fiber templates.After heat treatment,ZrO2 fiber mainly exists in monoclinic ZrO2 phase.With the increase of the heat treatment temperature,the grains in ZrO2 fibers become larger and the crystallinity degree increases,meanwhile the fiber surface undergoes a transition from smooth to small grains and then to cracks.

Key words: zirconia fiber, template impregnation method, micro-morphology, diameter

中图分类号: