耐火材料 ›› 2021, Vol. 55 ›› Issue (4): 325-328.DOI: 10.3969/j.issn.1001-1935.2021.04.012

• 生产应用 • 上一篇    下一篇

高性能转炉出钢口管砖的开发与应用

蔡长秀1)(), 雷中兴1), 徐小峰2,3), 周辉1), 李亚伟2,3), 朱天彬2,3)   

  1. 1)武钢耐火材料有限责任公司 湖北武汉 430080
    2)武汉科技大学 省部共建耐火材料与冶金国家重点实验室 湖北武汉 430081
    3)武汉科技大学 高温材料与炉衬技术国家地方联合工程研究中心 湖北武汉 430081
  • 收稿日期:2020-12-08 出版日期:2021-08-15 发布日期:2021-08-22
  • 作者简介:蔡长秀:女,1981年生,硕士,工程师。E-mail: carlcaroline098@163.com

Development and application of high performance taphole pipe brick for converter

Cai Changxiu1)(), Lei Zhongxing1), Xu Xiaofeng2,3), Zhou Hui1), Li Yawei2,3), Zhu Tianbin2,3)   

  1. 1)Wugang Refractories Co.,Ltd.,Wuhan 430080,Hubei,China
  • Received:2020-12-08 Online:2021-08-15 Published:2021-08-22

摘要:

以电熔镁砂、鳞片石墨为主要原料制备了镁碳质转炉出钢口管砖,研究了不同的抗氧化剂(Al粉、Al粉+Si粉、Al粉+Si粉+CaB6粉)和碳源种类(鳞片石墨、造粒石墨和膨胀石墨)对其性能的影响。结果表明:1)复合添加Al粉+Si粉+CaB6粉,镁碳出钢口管砖的抗氧化性能、高温抗折强度显著改善;2)引入造粒石墨有利于镁碳出钢口管砖的抗热震性和抗氧化性能的改善,膨胀石墨的添加虽能够显著改善镁碳出钢口管砖的抗热震性,但却降低了材料的抗氧化性能;3)研制的转炉出钢口管砖在某钢厂转炉应用,平均使用寿命181次,比之前提高了45%,效果良好。

关键词: 出钢口管砖, 抗氧化性, 抗热震性, 造粒石墨

Abstract:

The influences of different antioxidants (Al powder,Al powder+Si powder,Al powder+Si powder+CaB6 powder) and carbon sources (flake graphite,granulated graphite,and expanded graphite) on the properties of taphole pipe bricks for converter prepared using fused magnesia,flake graphite as raw materials were investigated.The results show that:(1)the oxidation resistance and hot modulus of rupture of magnesia-carbon taphole pipe bricks are significantly improved when using Al powder+Si powder+ CaB6 powder;(2)the introduction of granulated graphite is beneficial for the improvement of thermal shock resistance and oxidation resistance;although the addition of expanded graphite can significantly improve the thermal shock resistance,it reduces their oxidation resistance;(3)the developed taphole pipe bricks were applied in the converters in a steel plant with the average service life of 181 cycles,enhancing by 45%.

Key words: taphole pipe brick, oxidation resistance, thermal shock resistance, granulated graphite