耐火材料 ›› 2022, Vol. 56 ›› Issue (5): 391-395.DOI: 10.3969/j.issn.1001-1935.2022.05.005

• 研究开发 • 上一篇    下一篇

煤矸石陶粒替代闭孔珍珠岩骨料制备轻质铝硅系浇注料

昝文宇1), 马北越1), 王玉清2), 蒋志峰2)   

  1. 1)东北大学 冶金学院 辽宁沈阳 110819
    2)泰兴市恒信特种耐火材料有限公司 江苏泰州 225400
  • 收稿日期:2022-01-21 出版日期:2022-10-15 发布日期:2022-11-07
  • 作者简介:昝文宇:男,1996年生,硕士研究生。E-mail:1774299405@qq.com
  • 基金资助:
    2020年江苏省泰州市“双创计划”—创新人才资助项目(2020-18)。

Preparation of lightweight alumina-silica castables by replacing closed-cell perlite aggregates with coal gangue ceramsites

Zan Wenyu, Ma Beiyue, Wang Yuqing, Jiang Zhifeng   

  1. School of Metallurgy,Northeastern University,Shenyang 110819,Liaoning,China
  • Received:2022-01-21 Online:2022-10-15 Published:2022-11-07

摘要: 采用闭孔珍珠岩(粒度为2~4 mm)、开孔珍珠岩(粒度4~6 mm)和煤矸石陶粒(≤5 mm)为骨料,漂珠(0.3~0.5 mm)、沉珠(0.6~0.8 mm)、SiO2微粉、α-Al2O3微粉、氧化锆和锆英石微粉为细粉,Secar 71水泥(铝酸钙水泥)为结合剂制备了轻质铝硅系浇注料,研究了煤矸石陶粒加入量(加入质量分数分别为0、6%、12%、18%和24%)对制备轻质铝硅系浇注料性能的影响。结果表明:1)煤矸石陶粒的加入能降低试样的烧结收缩,提高其强度和抗热震性;2)加入煤矸石陶粒后的试样经过烧结后能够在基质中产生孔隙,为CA6复杂固溶体的生长提供足够空间,使不规则片状结构得到扩展;3)随着煤矸石陶粒加入量的增加,经1 000和1 200 ℃烧后试样的线收缩率先减小后增加,体积密度增加,显气孔率降低,经1 200 ℃烧后试样的常温耐压强度、抗热震性先增大后减小。综上,煤矸石陶粒适宜加入量为18%(w)。

关键词: 铝硅系浇注料, 闭孔珍珠岩, 煤矸石陶粒, 综合性能

Abstract: Lightweight alumina-silica castables were prepared using closed-cell perlite (2-4 mm),open-cell perlite (4-6 mm) and coal gangue ceramsites (≤5 mm) as aggregates,floating beads (0.3-0.5 mm),sinking beads (0.6-0.8 mm),silica micropowder,α-Al2O3 micropowder,zirconia and zircon micropowder as fines,and Secar 71 (calcium aluminate cement) cement as the binder.The effects of the coal gangue ceramsites addition (0,6%,12%,18% and 24%,by mass) on the properties of the as-prepared lightweight alumina-silica castables were investigated.The results show that:(1)the addition of coal gangue ceramsites can reduce the sintering shrinkage of the specimens and help to improve the strength and thermal shock resistance;(2)the specimens with the addition of coal gangue ceramsites can produce pores in the matrix of the sintered specimens,which provides enough space for the growth of CA6 complex solid solution and expands the irregular lamellar structure;(3)with the addition of coal gangue ceramsites increasing,the linear shrinkage of the specimens sintered at 1 000 or 1 200 ℃ firstly reduces and then increases,the bulk density increases and the apparent porosity decreases;the cold compression strength and the thermal shock resistance of the specimens sintered at 1 200 ℃ firstly increase and then decrease.Thus,the optimal addition of coal gangue ceramsites is 18%.

Key words: alumina-silica castables, closed-cell perlite, coal gangue ceramsites, comprehensive performance