耐火材料 ›› 2024, Vol. 58 ›› Issue (5): 440-444.DOI: 10.3969/j.issn.1001-1935.2024.05.014

• 生产应用 • 上一篇    下一篇

全氧燃烧玻璃窑用耐火材料抗碱蒸气侵蚀性研究

邓丽娜, 易帅, 薛飞, 潘传才, 许谦, 蒋晨, 白雅宁   

  1. 中国国检测试控股集团股份有限公司 北京 100024
  • 收稿日期:2024-03-21 出版日期:2024-10-15 发布日期:2024-10-16
  • 作者简介:邓丽娜:女,1992年生,硕士,工程师。E-mail:dengln221@163.com
  • 基金资助:
    北京市科技服务专项项目(YD-809)。

Alkali vapor corrosion resistance of refractories for oxy-fuel combustion glass furnace

Deng Lina, Yi Shuai, Xue Fei, Pan Chuancai, Xu Qian, Jiang Chen, Bai Yaning   

  1. China Testing & Certification International Group Co.,Ltd.,Beijing 100024,China
  • Received:2024-03-21 Online:2024-10-15 Published:2024-10-16

摘要: 采用坩埚法对全氧燃烧玻璃窑用优质硅砖、零膨胀硅砖、熔铸锆刚玉砖(AZS33)、α-β刚玉砖于1 600 ℃保温24 h进行了抗碱蒸气侵蚀性对比试验,并对侵蚀后试样进行了显微结构分析。结果表明:1)优质硅砖和零膨胀硅砖显气孔率较高,在高温碱蒸气条件下,硅砖中的钙硅氧化物和玻璃相不断析出滴落,持续溶解SiO2颗粒,抗碱蒸气侵蚀性差;2)熔铸锆刚玉砖在碱蒸气的作用下,产生较多的玻璃相,玻璃相滴落后留下气孔,但熔铸锆刚玉砖显气孔率低,碱蒸气侵蚀渗透慢,抗碱蒸气侵蚀性优良;3)α-β刚玉砖的玻璃相含量低,显气孔率低,碱蒸气侵蚀后骨架结构保持完整,抗碱蒸气侵蚀性更优;4)4种砖抗碱蒸气侵蚀性能的优劣顺序为:α-β刚玉砖>熔铸锆刚玉砖>零膨胀硅砖>优质硅砖。

关键词: 全氧燃烧, 抗碱蒸气侵蚀性, 优质硅砖, 零膨胀硅砖, 熔铸锆刚玉砖, α-β刚玉砖

Abstract: Crucible method was used to compare the alkali vapor corrosion resistance of high-quality silicon brick,zero expansion silicon brick,fused cast zirconia corundum brick (AZS33) and α-β corundum brick for oxy-fuel combustion glass furnace insulated at 1 600 ℃ for 2 h.The microstructures of the samples after corrosion were analyzed.The results show that:(1)high-quality silica bricks and zero-expansion silica bricks have higher apparent porosity,under high temperature and vapor conditions,calcium silicate oxides and glass phases continuously precipitate and drip,continuously melting SiO2 particles,resulting in poor resistance to vapor attack;(2)under the action of alkali vapor,fused cast zirconia corundum bricks produce more glass phases,which drip and form pores,however,the fused cast zirconia corundum bricks have low apparent porosity,the alkali vapor corrosion and penetration is slow,and the corrosion resistance to alkali vapor is excellent;(3)α-β corundum bricks have low glass phase content and low apparent porosity,after alkali vapor corrosion,the skeleton structure remains perfectly,which have stronger corrosion resistance to alkali vapor;(4)the alkali vapor resistance order of the four types of bricks is:α-β corundum brick>fused cast zirconia corundum brick>zero expansion silica brick>high-quality silica brick.

Key words: oxy-fuel combustion, alkali vapor corrosion resistance, high-quality silica brick, zero expansion silica brick, fused cast zirconia corundum brick, α-β corundum brick

中图分类号: