耐火材料 ›› 2021, Vol. 55 ›› Issue (1): 40-43.DOI: 10.3969/j.issn.1001-1935.2021.01.009

• 研究开发 • 上一篇    下一篇

煤熔渣对SiC-CA6复合材料的侵蚀机制分析

司瑶晨(), 夏淼, 孙红刚, 李红霞(), 杜一昊, 赵世贤, 尚心莲   

  1. 中钢集团洛阳耐火材料研究院有限公司 先进耐火材料国家重点试验室 河南洛阳 471039
  • 收稿日期:2020-05-19 出版日期:2021-02-15 发布日期:2021-02-15
  • 通讯作者: 李红霞,女,1965年生,博士,教授级高级工程师。E-mail: lihongx0622@l26.com
  • 作者简介:司瑶晨:男,1995年生,硕士。E-mail: 1650221915@qq.com
  • 基金资助:
    NSFC-河南联合基金重点支持项目(U1604252)

Corrosion mechanism analysis of coal slag on SiC-CA6 composites

Si Yaochen(), Xia Miao, Sun Honggang, Li Hongxia(), Du Yihao, Zhao Shixian, Shang Xinlian   

  1. State Key Laboratory of Advanced Refractories,Sinosteel Luoyang Institute of Refractories Research Co.,Ltd.,Luoyang 471039,Henan,China
  • Received:2020-05-19 Online:2021-02-15 Published:2021-02-15
  • Contact: Li Hongxia

摘要:

采用静态坩埚法,在埋碳气氛中对SiC-CA6复合材料进行了1 500 ℃保温3 h的抗煤熔渣侵蚀试验,通过XRD、SEM、EDS等分析了煤熔渣对SiC-CA6复合材料的侵蚀机制。结果表明:1)在还原气氛下,SiC-CA6复合材料中未发现明显的侵蚀层,形成的渗透层较薄且比较致密,表明SiC-CA6复合材料具有较好的抗煤熔渣性能。2)煤熔渣对SiC-CA6复合材料的侵蚀主要包括渣层界面处的SiC颗粒被渣中的铁氧化物氧化,以及基质中的CA6与渣中的SiO2、Al2O3、CaO反应生成CAS2。CAS2溶入渣中使得界面处局部区域内的熔煤渣黏度增大,抑制了熔渣向材料内部的进一步渗透。

关键词: SiC-CA6复合材料, 煤熔渣, 静态坩埚法, 侵蚀机制, 煤气化

Abstract:

The coal slag corrosion resistance of SiC-CA6 composites was tested using the static crucible method under carbon embedded atmosphere at 1 500 ℃ for 3 h.The corrosion mechanism of coal slag on SiC-CA6 composites was studied by means of XRD,SEM and EDS.The results show that:(1)in the reducing atmosphere,no obvious corrosion layer is found in the SiC-CA6 composites;the formed permeation layer is relatively thin and dense,indicating that SiC-CA6 composites have good slag corrosion resistance;(2)the corrosion mechanism of coal slag on SiC-CA6 composites mainly includes two aspects: the oxidation of SiC particles at the slag/sample interface by iron oxide in the slag and the reaction of CA6 in sample matrix with the SiO2,Al2O3 and CaO in the slag to form CAS2;the formed CAS2 can dissolve into the slag and increase the viscosity of the local slag at the slag/sample interface,therefore suppressing the further penetration of the slag into the material.

Key words: silicon carbide-CA6 composites, coal slag, static crucible method, corrosion mechanism, gasification