耐火材料 ›› 2021, Vol. 55 ›› Issue (6): 466-470.DOI: 10.3969/j.issn.1001-1935.2021.06.002

• 研究开发 • 上一篇    下一篇

养护湿度对铝酸钙水泥结合刚玉质浇注料性能的影响

李烨1,2)(), 陆昕昱3), 廖桂华1)(), 丁达飞1,2), 王青峰1), 张举2), 叶国田2)   

  1. 1)洛阳理工学院 材料科学与工程学院 河南洛阳 471023
    2)郑州大学 材料科学与工程学院 河南郑州 450001
    3)中国中化集团有限公司 创新与战略发展部 北京 100031
  • 收稿日期:2021-02-03 出版日期:2021-12-15 发布日期:2021-12-10
  • 通讯作者: 廖桂华,男,1961年生,博士,教授。E-mail: guihua.liao@163.com
  • 作者简介:李烨:男,1991年生,博士。E-mail: 850455005@qq.com
  • 基金资助:
    国家自然科学基金资助项目(51672255);武汉科技大学耐火材料与冶金重点实验室开放基金(G201604);武汉科技大学耐火材料与冶金重点实验室开放基金(G201403)

Effect of curing humidity on properties of calcium aluminate cement bonded corundum castables

Li Ye1,2)(), Lu Xinyu3), Liao Guihua1)(), Ding Dafei1,2), Wang Qingfeng1), Zhang Ju2), Ye Guotian2)   

  1. 1) School of Materials Science and Engineering,Luoyang Institute of Science and Technology,Luoyang 471023,Henan,China
  • Received:2021-02-03 Online:2021-12-15 Published:2021-12-10
  • Contact: Liao Guihua

摘要:

以板状刚玉、α-Al2O3微粉和铝酸钙水泥为原料制备刚玉质浇注料试样。将试样于25 ℃分别在不同的湿度养护3 d,再在110 ℃烘干24 h后分别于800、1 100、1 450和1 620 ℃保温3 h进行热处理,研究了养护湿度(40%、70%和100%)对其性能、物相组成、显微结构的影响。结果表明:随着养护湿度的降低,浇注料的脱模强度、烘干强度及中高温热处理后的常温抗折强度增大,而显气孔率及热震后的抗折强度保持率逐渐降低。另外,随着养护湿度降低,铝酸钙水泥的水化程度更高,1 620 ℃热处理后浇注料的骨料与基质结合更加紧密。

关键词: 养护湿度, 铝酸钙水泥, 刚玉质浇注料, 强度

Abstract:

Corundum based castables were prepared using tabular corundum,α-Al2O3 micropowder and calcium aluminate cement as starting materials,curing at 25 ℃ in different humidities for 3 d,drying at 110 ℃ for 24 h,and firing at 800,1 100,1 450 and 1 620 ℃ for 3 h,respectively.The effects of the curing humidity (40%,70%,and 100%) on the properties,the phase composition and the microstructure of the castables were researched.The results show that,as the curing humidity decreases,the demolding strength,the drying strength and the cold modulus of rupture of the samples increase while the apparent porosity and the MOR retention ratio decrease.Moreover,with the reduction of the curing humidity,the hydration degree of the calcium aluminate cement is enhanced,and the aggregates and the matrix are bonded more closely for the castable fired at 1 620 ℃.

Key words: curing humidity, calcium aluminate cement, corundum based castables, strength