耐火材料 ›› 2022, Vol. 56 ›› Issue (2): 141-145.DOI: 10.3969/j.issn.1001-1935.2022.02.010

• 研究开发 • 上一篇    下一篇

不同复合烧结助剂对气压烧结Si3N4陶瓷性能的影响

张创(), 宋仪杰()   

  1. 武汉科技大学 省部共建耐火材料与冶金国家重点实验室 湖北武汉 430081
  • 收稿日期:2021-04-23 出版日期:2022-04-15 发布日期:2022-04-21
  • 通讯作者: 宋仪杰,男,1949年生,博士,教授。E-mail: 1765031229@qq.com
  • 作者简介:张创:男, 1993年生,硕士研究生。E-mail: 773928583@qq.com

Influence of different composite sintering aids on properties of gas-pressure sintered Si3N4 ceramics

Zhang Chuang(), Song Yijie()   

  1. The State Key Laboratory of Refractories and Metallurgy,Wuhan University of Science and Technology,Wuhan 430081,Hubei,China
  • Received:2021-04-23 Online:2022-04-15 Published:2022-04-21
  • Contact: Song Yijie

摘要:

以Y2O3/Al2O3、Al2O3/MgO和Y2O3/Al2O3/MgO等为复合烧结助剂,研究烧结助剂类别及烧结温度(1 750、1 800、1 850 ℃)对气压烧结Si3N4陶瓷致密化、显微结构以及力学性能的影响。结果表明:以Y2O3/Al2O3为烧结助剂所制备样品的抗折强度、硬度和断裂韧性优于其他两种复合助剂制备试样的;Y2O3/Al2O3复合助剂有利于显微结构中高长径比β-Si3N4晶粒的形成。当烧结温度为1 800 ℃时,以Y2O3/Al2O3为烧结助剂样品的致密度和力学性能最优,此时体积密度为3.24 g·cm-3,线收缩率为20.73%,强度、硬度和断裂韧性达到最大值,分别为821.9 MPa、14.25 GPa和7.16 MPa·m1/2

关键词: Si3N4陶瓷, 烧结助剂, 力学性能, 显微结构

Abstract:

Effects of sintering aids and temperature (1 750 ℃,1 800 ℃,and 1 850 ℃) on densification,the mechanical properties and the microstructure of gas-pressure sintered Si3N4 ceramics were explored using Y2O3/Al2O3,Al2O3/MgO and Y2O3/Al2O3/MgO as composite sintering aids.The results show that the modulus of rupture,the hardness and the fracture toughness of the specimens prepared using Y2O3/Al2O3 as the sintering aid are better than those of the specimens using the other two aids,and the Y2O3/Al2O3 aid favors the formation of β-Si3N4 grains with high aspect ratio in the microstructures;when the sintering temperature is 1 800 ℃,the density and the mechanical properties of the specimens with Y2O3/Al2O3 as sintering aid are the best,the bulk density is 3.24 g·cm-3,and the linear shrinkage rate is 20.73%,with the highest strength,hardness,fracture toughness of 821.9 MPa,14.25 GPa and 7.16 MPa·m1/2,respectively.

Key words: silicon nitride ceramics, sintering aid, mechanical properties, microstructure