耐火材料 ›› 2021, Vol. 55 ›› Issue (4): 316-318.DOI: 10.3969/j.issn.1001-1935.2021.04.009

• 生产应用 • 上一篇    下一篇

MgO和Y2O3对气压烧结制备氮化硅陶瓷的影响

余冬玲1)(), 张会玲1,2), 罗宏斌1), 冯晓宇1), 吴南星1,2)()   

  1. 1)景德镇陶瓷大学 机械电子工程学院 江西景德镇 333403
    2)江西省陶瓷材料加工技术工程实验室 江西景德镇 333403
  • 收稿日期:2021-01-08 出版日期:2021-08-15 发布日期:2021-08-22
  • 通讯作者: 吴南星,男,1968年生,博士,教授。E-mail: ldhjdz1987@163.com
  • 作者简介:余冬玲:女,1987年生,硕士,副教授。E-mail: zhanghljs@163.com
  • 基金资助:
    国家自然科学基金资助项目(51964022)

Effects of MgO and Y2O3 on preparation of silicon nitride ceramics by gas pressure sintering

Yu Dongling1)(), Zhang Huiling1,2), Luo Hongbin1), Feng Xiaoyu1), Wu Nanxing1,2)()   

  1. 1)School of Mechanical and Electronic Engineering,Jingdezhen Ceramic Institute,Jingdezhen 333403,Jiangxi,China
  • Received:2021-01-08 Online:2021-08-15 Published:2021-08-22
  • Contact: Wu Nanxing

摘要:

分别添加不同量(质量分数分别为2%、4%、6%、8%、10%)的MgO粉或Y2O3粉作为烧结助剂,经球磨混合、造粒、成型、6 MPa氮气-1 750 ℃气压烧结制备氮化硅陶瓷,检测试样的相对密度,并分析其物相组成和显微结构。结果表明:1)MgO粉添加量为6%(w)的试样和Y2O3粉添加量为8%(w)的试样的相对密度分别达到其系列试样的最大值96.5%和98%。2)添加量相同时,添加Y2O3粉试样的相对密度均比添加MgO粉试样的大,表明Y2O3比MgO更能促进氮化硅陶瓷的烧结致密化。3)添加MgO粉或Y2O3粉均能促进α-Si3N4向 β-Si3N4 转变。

关键词: MgO, Y2O3, 氮化硅陶瓷, 气压烧结, 烧结致密度, 烧结助剂

Abstract:

Silicon nitride ceramics were prepared using different amounts of MgO or Y2O3 powder as sintering aids (2%,4%,6%,8%,and 10%),ball milling,granulating,shaping and sintering at 1 750 ℃ under 6 MPa nitrogen.The relative density of the specimens was determined,the phase composition and microstructure were explored.The results show that (1)the maximum relative density reached 96.5% or 98% with 6% MgO or 8% Y2O3,respectively;(2)with the same addition,the relative density of the sample with Y2O3 powder is higher than that with MgO powder,indicating that Y2O3 preforms better than MgO in promoting sintering densification;(3)MgO and Y2O3 powder both can promote the transition from α-Si3N4 to β-Si3N4.

Key words: magnesia, yttrium oxide, silicon nitride ceramics, gas pressure sintering, sintering densification, sintering aid