Refractories ›› 2025, Vol. 59 ›› Issue (6): 482-487.DOI: 10.3969/j.issn.1001-1935.2025.06.005

Previous Articles     Next Articles

Preparation of MgO-Mg2SiO4 refractories from light burnt magnesia and their thermal shock resistance

Wang Cairan, Hou Qingdong, Yu Jiayao, Gao Huinan, Bian Zuomin, Luo Xudong, He Xinye, Li Yihan   

  1. First author’s address:School of Materials and Metallurgy,University of Science and Technology Liaoning,Anshan 114051,Liaoning,China
  • Received:2025-03-14 Online:2025-12-15 Published:2025-12-23

利用中烧镁砂制备MgO-Mg2SiO4质耐火材料及抗热震性能研究

王采燃1), 侯庆冬1), 于佳瑶2), 高慧楠3), 边作民3), 罗旭东1,4), 何鑫叶5), 李一涵5)   

  1. 1)辽宁科技大学 材料与冶金学院 辽宁鞍山 114051
    2)鞍钢集团钢铁研究院 辽宁鞍山 114003
    3)鞍山钢铁集团耐火材料有限公司 辽宁鞍山 114000
    4)辽宁科技学院 辽宁本溪 117000
    5)辽宁铭轩新材料科技有限公司 辽宁鞍山 114200
  • 作者简介:王采燃:女,2000年生,硕士研究生。E-mail:2210316674@qq.com
  • 基金资助:
    辽宁省高校基本科研项目(LJ212510146021)。

Abstract: To solve the problems of wasting magnesite tailings resource and environmental pollution,medium burned magnesia prepared from magnesite tailings was selected as the raw material,adding SiO2 and Ca(OH)2 as additives to prepare MgO-Mg2SiO4 refractories at 1 450 ℃ for 3 h.The effects of SiO2 and Ca(OH)2 additions on the sintering and thermal shock resistance of the refractories were studied.The results show that the introduction of SiO2 and Ca(OH)2 jointly promotes the sintering of the material.When the additions of SiO2 and Ca(OH)2 are 1.96 mass% and 2.42 mass%,namely the molar ratio of Ca(OH)2 to SiO2 is 1,the sintering and thermal shock resistance of the sample are the optimal:the bulk density is 2.96 g·cm-3,the apparent porosity is 16.7%,the retention ratios of the cold modulus of rupture and cold compressive strength after thermal shock are 80% and 53%,respectively.The introduction of SiO2 and Ca(OH)2 also promotes the solid solution reaction between monticellite and forsterite,thus forming microcracks at the grain boundaries of the material.The cracks propagate and undergo deflection under stress,which plays a role in crack deflection toughening,thereby improving the thermal shock resistance of MgO-Mg2SiO4 refractories.

Key words: medium burned magnesia, MgO-Mg2SiO4 refractories, sintering performance, thermal shock resistance

摘要: 为了解决菱镁矿尾矿资源浪费及环境污染问题,选用菱镁矿尾矿制备的中烧镁砂为原料,以SiO2和Ca(OH)2为添加剂,经1 450 ℃保温3 h制备MgO-Mg2SiO4质耐火材料,研究了SiO2和Ca(OH)2对MgO-Mg2SiO4质耐火材料烧结性能及抗热震性能的影响。结果表明,SiO2和Ca(OH)2的引入共同促进了材料的烧结,当SiO2添加量为1.96%(w),Ca(OH)2添加量为2.42%(w),即添加剂Ca(OH)2、SiO2物质的量比为1时,试样的烧结性能与抗热震性能最佳,此时试样的体积密度和显气孔率分别为2.96 g·cm-3和16.7%,其热震后的抗折强度保持率与耐压强度保持率分别为80%和53%。SiO2和Ca(OH)2的引入也会促进钙镁橄榄石和镁橄榄石发生固溶反应,使材料晶界上出现微裂纹,应力作用下裂纹扩展并发生方向偏转,起到裂纹偏转增韧的效果,从而改善了MgO-Mg2SiO4质耐火材料的抗热震性能。

关键词: 中烧镁砂, MgO-Mg2SiO4质耐火材料, 烧结性能, 抗热震性能

CLC Number: