耐火材料 ›› 2026, Vol. 60 ›› Issue (5): 389-396.DOI: 10.3969/j.issn.1001-1935.2026.05.004

• 研究开发 • 上一篇    下一篇

纳米氧化锆对莫来石-刚玉浇注料显微结构和性能的影响

李世恩1,2), 陈平安1,2), 乔梦珂1,2), 朱颖丽1,2), 陈浮1,2), 吴江1,2), 罗港涛1,2), 李享成1,2)   

  1. 1)武汉科技大学 先进耐火材料全国重点实验室 湖北武汉 430081
    2)武汉科技大学 高温电磁材料与结构教育部重点实验室 湖北武汉 430081
  • 收稿日期:2025-10-22 出版日期:2026-10-15 发布日期:2026-10-29
  • 通讯作者: 陈平安,男,1986年生,博士,教授。E-mail:pinganchen@wust.edu.cn
  • 作者简介:李世恩:男,2001年生,硕士研究生。E-mail:19103769627@163.com
  • 基金资助:
    国家重点研发计划(2024YFB3714600)。

Effects of nano-zirconia on microstructure and properties of mullite-corundum castables

Li Shien, Chen Ping’an, Qiao Mengke, Zhu Yingli, Chen Fu, Wu Jiang, Luo Gangtao, Li Xiangcheng   

  1. First author’s address:State Key Laboratory of Advanced Refractories,Wuhan University of Science and Technology,Wuhan 430081,Hubei,China
  • Received:2025-10-22 Online:2026-10-15 Published:2026-10-29

摘要: 为提升莫来石-刚玉浇注料的高温力学强度,满足其在高温工业中的应用性与可靠性,以电熔莫来石为骨料,刚玉粉和α-Al2O3粉为细粉,ρ-Al2O3粉和铝酸盐水泥为结合剂,外加纳米ZrO2为改性剂,制备莫来石-刚玉浇注料。研究纳米ZrO2添加量(加入质量分数分别为0、0.4%、0.8%、1.2%、1.5%、2.0%和3.0%)对浇注料显微结构和性能的影响。结果表明:纳米ZrO2分散在浇注料基质中,促进了六铝酸钙(CA6)晶粒的形核和长大;随着纳米ZrO2添加量的增加,板片状CA6生成量增多,且交错分布在基质中;与未添加纳米ZrO2的浇注料相比,添加2.0%(w)纳米ZrO2的莫来石-刚玉浇注料的力学性能最好,添加0.8%(w)纳米ZrO2的莫来石-刚玉浇注料的抗热震性和抗渣侵蚀性最好。

关键词: 莫来石-刚玉浇注料, 纳米ZrO2, CA6, 高温抗折强度, 抗侵蚀性能

Abstract: To enhance their hot mechanical strength and satisfy their applicability and reliability in high-temperature industries,mullite-corundum castables were prepared using fused mullite as aggregates,corundum powder and α-Al2O3 powder as fine powders,ρ-Al2O3 powder and calcium aluminate cement as binders,and nano-ZrO2 as the modifier.The effects of the nano-ZrO2 additions (0,0.4%,0.8%,1.2%,1.5%,2.0%,and 3.0%,by mass) on the microstructure and properties of the castables were investigated.The results show that nano-ZrO2 is dispersed in the matrix of the castables and promotes the nucleation and growth of calcium hexaluminate (CA6) grains.With the increase of the nano-ZrO2 addition,the amount of plate-like CA6 increases,and CA6 exhibits interlocking distribution in the matrix.Compared with the castable without nano-ZrO2,the one with 2.0% nano-ZrO2 demonstrates the optimal mechanical properties,while the one with 0.8% nano-ZrO2 shows the best thermal shock resistance and slag corrosion resistance.

Key words: mullite-corundum castables, nano-ZrO2, calcium hexaaluminate, hot modulus of rupture, corrosion resistance